Induction Hardening Teeth Of Gear
Views Send Enquiry
Objective Hardening teeth on a steel motorcycle gear to a hardness of 48 – 55 HRC
Material Carbon steel gear 6.9” (175mm) diameter
Temperature 2000 ºF ( 1093 ºC)
Frequency 78 kHz
Equipment •Power of 90 kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 8μF
• An induction heating coil designed and developed specifically for this application.
Process A single turn helical coil is used to heat the gear. The gear is placed on a spindle and rotated at 300-350 RPM’s. Heat is applied for 10 seconds to reach the desired hardness. The gear is immediately quenched to remove the heat, dried and then coated with a lubricant.
Results/Benefits Induction heating provides:
• Easy control of depth of hardness
• Energy savings due to efficiency of process
• Hands-free heating that involves no operator skill for manufacturing
• Even distribution of heating
hardening-gear-teech
Related Content
Air Cooled clamp coil (half-open coil) for preheating gas pipeline
induction coating by air cooled clamp induction coil
Remove plastic coating from steel tubes by Induction Heating
Releasing Fixture by Induction Heating
U shape air cooled induction coil by UM-100C-HF for pipeline preheating
induction quenching with custom-design inductor
induction brazing diamond segment
induction brass soldering copper plate_2
Hot
induction hardening axle (shaft) by 100KW induction heater
induction quenching axle (shaft) by 160KW induction heater
induction hardening inner surface (inwall)
Induction Hardening Harvestor Combined Finger
Induction Hardening Harvestor Combined Blade
workpiece for induction hardening
induction hardening veterinary instrument
induction hardening surgical device
Newest Comment
No Comment
Post Comment